New Test Method 106.3.2.101, Chemical analysis on Loss on Ignition (LOI) ignited aggregates and other materials 

106.3.2.101 TM 101, Chemical analysis on Loss on Ignition (LOI) ignited aggregates and other materials

106.3.2.101.1 Scope

Concrete aggregates, such as limestones and dolomites, usually contain high carbonate (calcium and magnesium) concentrations. This makes it extremely difficult to achieve complete fusion of sample(s) using a lithium metaborate (LiBO2) flux and dissolving the fused pellet in a weak nitric acid solution. By running the LOI, moisture and carbon dioxide (CO2), can be removed and the remaining inorganic residue can be adjusted to allow for better dissolution of sample(s).

106.3.2.101.2 Equipment

Platinum crucible, 20-ml capacity used only for aggregates

Porcelain crucible, 15-ml capacity used only for fly ash and natural pozzolans

Muffle furnace, 1000 degrees C temperature capacity

Spatula, approximately 6 inches in length

Analytical balance, capable of weighing 4 places past the decimal point

Inductively Couple Plasma Optical Emmission Spectrometer (ICP-OES)

Graphite crucible, used to fuse sample with a bed of LiBO2 contained in the crucible

Lithium metaborate (LiBO2), ACS anhydrous grade

Nitric acid (HNO3), certified ACS plus grade

Yttrium (Y), 1000 ppm liquid standard, 250-ml

¼ teaspoon, leveling knife and test tube with same diameter of the graphite crucible to fuse sample

Polypropylene beaker, 250-ml capacity

Filter paper, ashless #41, 110 mm diameter

Glass filter funnel

200-ml volumetric flask with graduated mark


106.3.2.101.3 Method

Obtain a clean, dry platinum crucible and weigh on an analytical balance. Record the weight to 4 places past the decimal point. Add 1 gram of sample to the initial weight of the crucible and record. Weigh sample to initial weight plus 1 gram in the platinum crucible to +/- 0.0005. Place crucible and sample contents into a cool muffle furnace. Bring temperature to 1000 degrees C (+/- 50 degrees) and keep in muffle furnace for 2 hours. After 2 hours, carefully remove crucible with tongs and place in desiccator to cool. Once crucible is cool, weigh to constant weight and record weight.

Place a ¼ teaspoon of LiBO2 into a graphite crucible and press down using a test tube to make a bed of LiBO2. Weigh LOI ignited material from the example calculation listed below and cover sample with a ¼ teaspoon of LiBO2 to encapsulate sample. Using tongs, place graphite crucible in a 1000 degree C muffle furnace for 20 minutes. After 20 minutes, carefully remove graphite crucible with tongs, swirl fused bead to obtain any fused particles indirect of the fused bead, and drop fused bead directly into a polypropylene beaker containing 150-ml 1:24 HNO3. Using a spatula, carefully scrape any remaining residue left in the graphite crucible and transfer to beaker. Place beaker on stir plate for a minimum of 5 minutes. Set-up filter funnel with a #41 filter paper and place 200-ml volumetric flask with 1-ml Yttrium added to the flask. Remove beaker from stir plate and filter into 200-ml volumetric flask. The filter removes any carbon from the solution. Quantitatively wash beaker twice with 1:24 HNO3 and dilute to volume. Analyze for selected analytes in solution using existing test template set in the ICP-OES software for aggregate analysis.

106.3.2.101.4 Calculation

Initial weight – final weight x 100 = % LOI

Once LOI has been determined, adjust weight of 0.2 +/- 0.0005 to LOI result and record.

Example: If % LOI is 42.00, subtract 100-42.00 = 58.00, multiply 0.2 +/- 0.0005 x .58 = 0.116 grams. This is the LOI corrected weight to fuse with LiBO2.

Perform the same method for standards and use the same test template on the ICP-OES to obtain concentration of selected analytes in solution

Note: This method can be used on other materials, such as high carbon Class C, F ashes, and natural pozzolans.

106.3.2.101.5 Synopsis

By removing the moisture and CO2, samples can be fused, dissolved, and the proper % recovery of the sample can be achieved.